With the cowl top side upper panel assembly removed.
REMOVAL
| Symbol Meaning | |
|---|---|
|
Remove Weld Points |
|
Cut and Join Location |
|
Cut Location for Supply Parts |
Do not butt weld or heat repair because the heat decreases the strength of areas where ultra high strength steel is used. (See the introduction)
Roughly cut open the panel so that the adhesive can be reached. Cut through the adhesive with a cut chisel to remove the panel.
In cases where the adhesive cannot be removed with a cut chisel, heat the adhesive with an industrial heater gun or gas burner taking care not to cause panel deformation by overheating.
|
Adhesive | - | - |
Remove the side member assembly.
| *1 | SIDE MEMBER ASSEMBLY | - | - |
| *a | 30 mm (1.18 in.) | - | - |
Roughly cut open the panel so that the adhesive can be reached. Cut through the adhesive with a cut chisel to remove the panel.
In cases where the adhesive cannot be removed with a cut chisel, heat the adhesive with an industrial heater gun or gas burner taking care not to cause panel deformation by overheating.
|
Adhesive | - | - |
Remove the A.
When replace only the outer panel, please cut off a necessary range depending on a damage range.
Carefully cut the outer panel so not to damage the reinforcement.
Make sure that butt welding does not heat-affect the reinforcement when welding the outer panel.
INSTALLATION
| Symbol Meaning | |
|---|---|
|
Remove Weld Points |
|
Plug Weld |
|
Butt Weld |
|
Body Sealer |
Inspect the fitting of the related parts around the new parts before welding. This affects the appearance of the finish.
Temporarily install the new parts and measure each part of the new parts in accordance with the body dimension diagram. (See the body dimensions)
If the entire supply part is not needed, remove the part of the supply part that is needed.
| *1 | FRONT PILLAR REINFORCEMENT SUB-ASSEMBLY LOWER | - | - |
Apply adhesive (3MTM AutomixTM Panel Bonding Adhesive #8115).
Do not apply adhesive around the plug welding points.
Minimize squeeze out in plug welding areas.
|
Adhesive | - | - |
Weld the A to the vehicle side.
When welding 2 panels together including 780 MPa ultra high strength steel.
| *a: Plug weld | Plug diameter | 10 mm (0.39 in.) |
| Wire type | AWS A5.18 ER70S-3 | |
| Shield gas | Metal active gas |
Be sure to use Metal active gas (Ar 80% + CO2 20%) as the shield gas when plug welding.Sufficient weld strength cannot be assured when using 100% CO2 shield gas.
Before installing a new part, apply body sealer.
Apply body sealer in an even, continuous bead.
Apply adhesive (3MTM AutomixTM Panel Bonding Adhesive #8115).
Do not apply adhesive around the plug welding points.
Minimize squeeze out in plug welding areas.
|
Adhesive | - | - |
Weld the side member assembly.
| *1 | SIDE MEMBER ASSEMBLY | - | - |
When welding 3 panels or more together including 780 MPa ultra high strength steel. (When plug welding a third panel to 2 panels which are welded under the conditions described above.)
| *a: Plug weld | Plug diameter | Same as the standard method (See the introduction) |
| Wire type | AWS A5.18 ER70S-3 | |
| Shield gas | Metal active gas |
Be sure to use Metal active gas (Ar 80% + CO2 20%) as the shield gas when plug welding.Sufficient weld strength cannot be assured when using 100% CO2 shield gas.
When welding 3 panels or more together including 780 MPa ultra high strength steel. (When plug welding a third panel to 2 panels which are welded under the conditions described above.)
| *a: Plug weld | Plug diameter | Same as the standard method (See the introduction) |
| Wire type | AWS A5.18 ER70S-3 | |
| Shield gas | Metal active gas |
Be sure to use Metal active gas (Ar 80% + CO2 20%) as the shield gas when plug welding.Sufficient weld strength cannot be assured when using 100% CO2 shield gas.
After welding, apply body sealer to the corresponding parts. (See the painting/coating)
After applying the top coat, apply anti-rust agent to the internal panel portion of the closed section structural weld points.