With the quarter panel assembly removed.
REMOVAL
| Symbol Meaning | |
|---|---|
|
Remove Weld Points |
|
Remove Weld Points |
|
Cut and Join Location |
Do not butt weld or heat repair because the heat decreases the strength of areas where ultra high strength steel is used. (See the introduction)
Remove the A.
A is reused.
| *a | 105 mm (4.13 in.) | *b | 265 mm (10.43 in.) |
| *c | 20 mm (0.79 in.) | - | - |
Roughly cut open the panel so that the adhesive can be reached. Cut through the adhesive with a cut chisel to remove the panel.
In cases where the adhesive cannot be removed with a cut chisel, heat the adhesive with an industrial heater gun or gas burner taking care not to cause panel deformation by overheating.
|
Adhesive | - | - |
Remove the center body pillar reinforcement sub-assembly.
| *1 | CENTER BODY PILLAR REINFORCEMENT SUB-ASSEMBLY | - | - |
Remove the center body pillar reinforce sub-assembly lower.
| *1 | CENTER BODY PILLAR REINFORCE SUB-ASSEMBLY LOWER | - | - |
| *a | 50 mm (1.97 in.) | *b | 45 mm (1.77 in.) |
INSTALLATION
| Symbol Meaning | |
|---|---|
|
Spot Weld |
|
Plug Weld |
|
Plug Weld |
|
Butt Weld |
Inspect the fitting of the related parts around the new parts before welding. This affects the appearance of the finish.
Temporarily install the new parts and measure each part of the new parts in accordance with the body dimension diagram. (See the body dimensions)
Weld the center body pillar reinforce sub-assembly lower to the vehicle side.
| *1 | CENTER BODY PILLAR REINFORCE SUB-ASSEMBLY LOWER | - | - |
Apply adhesive (3MTM AutomixTM Panel Bonding Adhesive #8115).
Do not apply adhesive around the plug welding points.
Minimize squeeze out in plug welding areas.
|
Adhesive | - | - |
Weld the center body pillar reinforcement sub-assembly to the vehicle side.
| *1 | CENTER BODY PILLAR REINFORCEMENT SUB-ASSEMBLY | - | - |
| *a | Ultra High Strength Steel Welding Point | *b | Ultra High Strength Steel Welding Point |
When welding 2 panels together including 980 MPa ultra high strength steel.
| *a: Spot weld | Pressure | 2940 N (300 kgf, 661 lbf) |
| Weld current | 10000 A | |
| Weld time | 18 Cyc.(0.34 Sec.) | |
| *b: Plug weld | Plug diameter | 10 mm (0.39 in.) |
| Wire type | AWS A5.18 ER70S-6/ER70S-3 | |
| Shield gas | Metal active gas |
Be sure to use Metal active gas (Ar + CO2 20 to 30% or Ar + O2 2%) as the shield gas when plug welding. Sufficient weld strength cannot be assured when using 100% CO2 shield gas.
Weld the A to the vehicle side.
| *a | Ultra High Strength Steel Welding Point | - | - |
When welding 3 panels or more together including 980 MPa ultra high strength steel. (When plug welding a third panel to 2 panels which are welded under the conditions described above.)
| *a: Plug weld | Plug diameter | Same as the standard method (See the introduction) |
| Wire type | AWS A5.18 ER70S-6/ER70S-3 | |
| Shield gas | Metal active gas |
Be sure to use Metal active gas (Ar + CO2 20 to 30% or Ar + O2 2%) as the shield gas when plug welding. Sufficient weld strength cannot be assured when using 100% CO2 shield gas.
After welding, apply the foamed sealing material to the corresponding parts. (See the painting/coating)
After applying the top coat, apply anti-rust agent to the internal panel portion of the closed section structural weld points.